A study of four commercial natural colorants in two biodegradable polyesters has found that most formulations can be compounded and injection molded on conventional equipment without major processing or mechanical penalties, but that long-term color stability remains the main obstacle to wider use.
The work, titled “Sustainability in the Development of Natural Pigment-Based Colour Masterbatches and Their Application in Biopolymers,” combined blue spirulina, yellow curcumin, red beetroot and green chlorophyllin with polylactic acid (PLA) and polybutylene succinate (PBS). Masterbatches were produced by twin-screw extrusion, let down into the matching polymer matrix at 2, 4 and 6 wt%, and molded into test specimens. The formulations also contained titanium dioxide, calcium carbonate and stearic acid to support UV protection, dispersion and processing.
Thermal window sets the limits
Thermogravimetric analysis placed the onset of degradation at roughly 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot, all below the degradation temperatures of the two matrices. The researchers therefore selected profiles that melted each polymer while limiting the pigments' heat exposure: 145 °C for PBS and 190 °C for PLA, with the twin-screw extruder running at 65 rpm and a feed rate of 2 kg/h.
That window suited most pigment–polymer pairs, but spirulina was the notable exception. During PLA processing it lost its characteristic blue, and a blue PLA masterbatch could not be produced. In PBS, whose lower processing temperature kept the pigment sufficiently stable, compounding succeeded. The result indicates that pigment compatibility depends strongly on the thermal requirements of the matrix, not on the colorant alone.
Flow and mechanics stay close to baseline
Rheology changed only modestly. Neat PLA showed a melt flow rate of about 50 g/10 min, and the natural-pigment masterbatches remained near that value; PBS responded similarly, with a small reduction in MFR that points to a slight rise in melt viscosity. The authors note this matters for compounders, since a color system that forced changes to screw design, pressure settings or molding conditions would offer little practical value.
Tensile and impact behavior stayed close to the uncolored baselines across the 2–6 wt% range. PLA started at a Young's modulus of about 1710 MPa and tensile strength of 65.6 MPa; PBS started at about 392 MPa and 34.5 MPa. Impact strength also remained in a comparable range, although individual pigments introduced some variation.
Photostability is the weak point
Successful extrusion did not translate into durable color. After 50 hours of xenon-lamp exposure, most formulations exceeded a color difference of ΔE* = 2, the level at which a change becomes visually perceptible. The clearest exception was PLA containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.
The study identifies UV stability as the largest barrier to broader adoption. Packaging, consumer products, agricultural parts and outdoor applications would likely need additional stabilization, protective coatings or pigment modification before natural colors could compete with conventional systems over long service periods.
Lower footprint, unfinished performance
Under the study's assumptions, the environmental comparison favored the bio-based colorants: one kilogram of curcumin pigment corresponded to about 0.04 kg CO2-eq, against 18.65 kg CO2-eq for the inorganic green reference pigment, and the natural-pigment masterbatches also consumed less electricity during extrusion and pelletizing.
The authors conclude that further development is needed, particularly in lightfastness and thermal stability, but that several natural colorants can be compounded into PLA and PBS on standard processing equipment with only limited changes in melt viscosity and mechanical performance. Future work, they suggest, should target color stability both during processing and during subsequent service exposure.